Heerka fulinta | ZEICIN darajada | GB | AISI | JIS | DIN |
---|---|---|---|---|---|
GB/T9943-2008 | M2 | W6Mo5Cr4V2 | M2 | SKH51 | 1.3343 |
ASTM A681 | C | Si | Mn | P | S | Cr | Mo | V | W |
M2/ T11302 | 0.78~0.88 | 0.20~0.45 | 0.15~0.40 | 0.030 Max | 0.030 Max | 3.75~4.50 | 4.50~5.50 | 1.75~2.20 | 5.50~6.75 |
DIN 17350 | C | Si | Mn | P | S | Cr | Mo | V | W |
1.3343 / S6-5-2 | 0.86~0.94 | ≤0.45 | ≤0.40 | 0.030 Max | 0.030 Max | 3.80~4.50 | 4.70~5.20 | 1.70~2.00 | 6.00~6.70 |
GB/T 9943 | C | Si | Mn | P | S | Cr | Mo | V | W |
W6Mo5Cr4V2 | 0.80~0.90 | 0.20~0.45 | 0.15~0.40 | 0.030 Max | 0.030 Max | 3.80~4.40 | 4.50~5.50 | 1.75~2.20 | 5.50~6.75 |
JIS G4403 | C | Si | Mn | P | S | Cr | Mo | V | W |
SKH51/SKH9 | 0.80~0.88 | ≤0.45 | ≤0.40 | 0.030 Max | 0.030 Max | 3.80~4.50 | 4.70~5.20 | 5.90~6.70 | 1.70~2.10 |
Adag, Rockwell C (ku kululaaday 621°C, demiyay 1204°C): 62 HRC.
Adag, Rockwell C (deminta 1204°C)): 65 HRC
Laga been abuurtay M2 HSS Biraha birta ahMarka hore, Pre-kuleylka ilaa 650-750 ℃, ka dibna kulayl heerkul been abuur ah. Ku qooya 1204°C, hubi kulaylka si fiican. Ka dibna billow foornada, heerkulka foornada oo aan ka yarayn 950 ℃. Ka dib markii la been abuurtay, si tartiib ah u qabooji.
Marka hore, si tartiib ah u kululee ilaa 871 ℃, ka dibna si tartiib ah u qabooji 538 ℃ (1000 ℉) foornada daaweynta kulaylka. Kadibna ku qabooji hawada. Ka dib markii la tirtiray adkaanta HBS: 255 Max.
Birta M2 oo leh adkeysi aad u sarreeya waana in lagu adkeeyaa iyadoo lagu qaboojinayo hawada weli jirta. Isticmaalka qubeyska milixda ah ama foornada jawiga la xakameeyey ayaa la jecel yahay si loo yareeyo decarburization, iyo haddii aan la heli karin, baakad adag oo ku jirta kookaha la isticmaalay ayaa la soo jeediyay.
Heerkulka Demiyey / ℃ | foornada qubeyska milixda: 1204
Heerkulka Demiyey / ℃ | foornada jawiga la xakameeyey: 1216
Waqtiga ilaalinta kulaylka /daqiiqo: 5 ~ 15
Dhexdhexaadinta deminta: qaboojinta saliidda
Adag: 65 HRc Min
Heerkulka heerkulka / ℃ : 540-564