Baja tahan karat 347/ 347H BUSHING
Stainless Steel 347/ 347H TEE
Bobot % (kabeh nilai maksimal kajaba ana sawetara sing dituduhake)
unsur | 347 | 347H |
Kromium | 17.00 min.-19.00 maks. | 17.00 min.-19.00 maks. |
nikel | 9.00 min.-13.00 maks. | 9.00 min.-13.00 maks. |
Karbon | 0.08 | 0.04 min.-0.10 maks. |
Mangan | 2.00 | 2.00 |
Fosfor | 0.045 | 0.045 |
belerang | 0.03 | 0.03 |
silikon | 0.75 | 0.75 |
Columbium & Tantalum | 10 x (C + N) min.-1,00 maks. | 8 x (C + N) min.-1.00 maks. |
wesi | imbangan | imbangan |
SIFAT FISIK
Kapadhetan: 0,288 lbs/in3 7,97 g/cm3 Tahanan Listrik: mikrohm-in (mikrohm-cm): 68 °F (20 °C): 28,7 (73)
Kalor Spesifik: BTU/lb/°F (kJ/kg•K):
32 - 212 °F (0 - 100 °C): 0,12 (0,50)
Konduktivitas Termal: BTU/hr/ft2/ft/°F (W/m•K):
Ing suhu 212 °F (100 °C): 9.3 (16.0)
Ing 932 °F (500 °C): 12.8 (22.0)
Rata-rata Koefisien Ekspansi Termal: ing/in/°F (µm/m•K):
32 - 212 °F (0 - 100 °C): 9,3 x 10·6 (16,6)
32 - 1000 °F (0 - 538 °C): 10,5 x 10·6 (18,9)
32 - 1500 °F (0 - 873 °C): 11,4 x 10·6 (20,5)
Modulus elastisitas: ksi (MPa):
28 x 103 (193 x 103) ing tension
11 .2 x 103 (78 x 103) ing torsi
Permeabilitas Magnetik: H = 200 Oersteds: Annealed < 1,02 maks.
Rentang lebur: 2500 - 2550 °F (1371 - 1400 °C)