Utfiering Standert | ZEICIN Grade | GB | AISI | JIS | DIN |
---|---|---|---|---|---|
GB/T9943-2008 | M2 | W6Mo5Cr4V2 | M2 | SKH51 | 1.3343 |
ASTM A681 | C | Si | Mn | P | S | Cr | Mo | V | W |
M2/ T11302 | 0.78~0.88 | 0.20~0.45 | 0.15~0.40 | 0.030 Max | 0.030 Max | 3.75~4.50 | 4.50~5.50 | 1.75~2.20 | 5.50~6.75 |
DIN 17350 | C | Si | Mn | P | S | Cr | Mo | V | W |
1.3343/ S6-5-2 | 0.86~0.94 | ≤0,45 | ≤0,40 | 0.030 Max | 0.030 Max | 3.80~4.50 | 4.70~5.20 | 1.70~2.00 | 6.00~6.70 |
GB/T 9943 | C | Si | Mn | P | S | Cr | Mo | V | W |
W6Mo5Cr4V2 | 0.80~0.90 | 0.20~0.45 | 0.15~0.40 | 0.030 Max | 0.030 Max | 3.80~4.40 | 4.50~5.50 | 1.75~2.20 | 5.50~6.75 |
JIS G4403 | C | Si | Mn | P | S | Cr | Mo | V | W |
SKH51/SKH9 | 0.80~0.88 | ≤0,45 | ≤0,40 | 0.030 Max | 0.030 Max | 3.80~4.50 | 4.70~5.20 | 5.90~6.70 | 1.70~2.10 |
Hurdens, Rockwell C (tempered by 621 ° C, quenched by 1204 ° C): 62 HRC.
Hurdheid, Rockwell C (blust by 1204 ° C)): 65 HRC
Smeden fan M2 HSS Steel metaal materiaalEarst, Pre-heating nei 650-750 ℃, dan ferwaarmje nei smeid temperatuer. Soak op 1204 ° C, soargje foar waarmte. Dan begjinne smeid, de smeid temperatuer net leech dan 950 ℃. Nei it smeden, koelje stadichoan.
Earst, stadich ferwaarmje oant 871 ℃, dan stadich koelje oant 538 ℃ (1000 ℉) yn waarmtebehannelingofen. Dan koelje yn 'e loft. Nei annealing hurdens HBS: 255 Max.
M2 stiel hawwende tige hege hardenability en moat wurde ferhurde troch koeling yn stille loft. It brûken fan in sâlt bad of kontrolearre atmosfear oven is winsklik te minimalisearje decarburization, en as net beskikber, pack ferhurding yn bestege pitch coke wurdt suggerearre.
Blustemperatuer / ℃ | sâlt bad oven: 1204
Blustemperatuer / ℃ | kontrolearre atmosfear oven: 1216
De waarmtebehâldtiid/min: 5 ~ 15
Quenching medium: oalje cooling
Hardheid: 65 HRc Min
Temperatuer temperatuer / ℃: 540-564
Nei tempering hurdens HRC of heger: 65 Min